Ordinary refractive index
Spread
Each mark is one record; bars are stated ranges, whiskers stated uncertainties. Filled marks: P, P-comp, P-db; hollow: S, V, C, P(abs). Hover a mark for its source. Each row has its own axis; no mean or fit is drawn.
Records
| Value | Unit | Variant | Conditions | Frame | Source | Locator | Status |
|---|---|---|---|---|---|---|---|
| 2.2321 default record | – | Congruent LiNbO3 (CLN) | T 21 °C; λ 1064 nm | – | Zelmon et al., Journal of the Optical Society of America B 14 3319 (1997) derived: evaluated from dispersion model Zelmon 1997 congruent, ordinary at 1064 nm, 21 C (rounded to 1e-4) | – | C |
| 2.2111 default record | – | Congruent LiNbO3 (CLN) | T 21 °C; λ 1550 nm | – | Zelmon et al., Journal of the Optical Society of America B 14 3319 (1997) derived: evaluated from dispersion model Zelmon 1997 congruent, ordinary at 1550 nm, 21 C (rounded to 1e-4) | – | C |
| 2.2865 default record | – | Congruent LiNbO3 (CLN) | T 21 °C; λ 632.8 nm | – | Zelmon et al., Journal of the Optical Society of America B 14 3319 (1997) derived: evaluated from dispersion model Zelmon 1997 congruent, ordinary at 632.8 nm, 21 C (rounded to 1e-4) | – | C |
| 2.2866 | – | Congruent LiNbO3 (CLN) | λ 632.8 nm | – | Crystal Technology, Inc. (1999) | – | V |
| Identical to Nelson & Mikulyak 1974. | |||||||
| 2.2323 | – | Congruent LiNbO3 (CLN) | T 24.5 °C; λ 1060 nm | – | Weis & Gaylord, Applied Physics A 37 191-203 (1985) original: Nelson & Mikulyak, J. Appl. Phys. 45, 3688 (1974) | Table 2, p. 197 | P-comp |
| 2.2866 | – | Congruent LiNbO3 (CLN) | T 24.5 °C; λ 632.8 nm | – | Weis & Gaylord, Applied Physics A 37 191-203 (1985) original: Nelson & Mikulyak, J. Appl. Phys. 45, 3688 (1974) | Table 2, p. 197 | P-comp |
| Weis & Gaylord 1985 Table 2 misprints n_o at 472.7 nm as 3.3597. | |||||||
| 2.1391 default record | – | LiTaO3, composition not stated (comparison material) 1965 bulk crystal | T room temperature; λ 1000 nm | – | Bond, Journal of Applied Physics 36 1674-1677 (1965) | refractiveindex.info LiTaO3/Bond-o tabulated data | P-db |
| n_e > n_o at every tabulated wavelength (0.45-4.0 um) in this dataset: LT is weakly positive uniaxial here, unlike LN. | |||||||
| 2.1174 default record | – | LiTaO3, composition not stated (comparison material) 1965 bulk crystal | T room temperature; λ 1600 nm | – | Bond, Journal of Applied Physics 36 1674-1677 (1965) | refractiveindex.info LiTaO3/Bond-o tabulated data | P-db |
| n_e > n_o at every tabulated wavelength (0.45-4.0 um) in this dataset: LT is weakly positive uniaxial here, unlike LN. | |||||||
| 2.1834 default record | – | LiTaO3, composition not stated (comparison material) 1965 bulk crystal | T room temperature; λ 600 nm | – | Bond, Journal of Applied Physics 36 1674-1677 (1965) | refractiveindex.info LiTaO3/Bond-o tabulated data | P-db |
| n_e > n_o at every tabulated wavelength (0.45-4.0 um) in this dataset: LT is weakly positive uniaxial here, unlike LN. | |||||||
| 2.2288 default record | – | 5 mol% MgO-doped congruent LiNbO3 (MgO5) | T 21 °C; λ 1064 nm | – | Zelmon et al., Journal of the Optical Society of America B 14 3319 (1997) derived: evaluated from dispersion model Zelmon 1997, 5 mol% MgO:congruent LN, ordinary (erratum applied) at 1064 nm, 21 C (rounded to 1e-4) | – | C |
| 2.2082 default record | – | 5 mol% MgO-doped congruent LiNbO3 (MgO5) | T 21 °C; λ 1550 nm | – | Zelmon et al., Journal of the Optical Society of America B 14 3319 (1997) derived: evaluated from dispersion model Zelmon 1997, 5 mol% MgO:congruent LN, ordinary (erratum applied) at 1550 nm, 21 C (rounded to 1e-4) | – | C |
| 2.2825 default record | – | 5 mol% MgO-doped congruent LiNbO3 (MgO5) | T 21 °C; λ 632.8 nm | – | Zelmon et al., Journal of the Optical Society of America B 14 3319 (1997) derived: evaluated from dispersion model Zelmon 1997, 5 mol% MgO:congruent LN, ordinary (erratum applied) at 632.8 nm, 21 C (rounded to 1e-4) | – | C |
| 2.288 default record | – | Stoichiometric or near-stoichiometric LiNbO3 (SLN) near-stoichiometric | λ 633 nm | – | Volk & Wöhlecke, Springer Series in Materials Science 115 (2009) | Table 1.2, p. 4 (refs. [26-28]) | P-comp |
| 2.291 | – | Stoichiometric or near-stoichiometric LiNbO3 (SLN) labelled 'stoichiometric' (1967 crystal) | T 25 °C; λ 632.8 nm | – | Weis & Gaylord, Applied Physics A 37 191-203 (1985) original: Boyd, Bond, Carter, J. Appl. Phys. 38, 1941 (1967) | Table 2, p. 197 | P-comp |
| Conflicts with Volk & Wöhlecke 2009 near-SLN values. | |||||||
Congruent LiNbO3 (CLN)
CCongruent LiNbO3 (CLN)
CCongruent LiNbO3 (CLN)
VIdentical to Nelson & Mikulyak 1974.
Congruent LiNbO3 (CLN)
P-compCongruent LiNbO3 (CLN)
P-compWeis & Gaylord 1985 Table 2 misprints n_o at 472.7 nm as 3.3597.
LiTaO3, composition not stated (comparison material)1965 bulk crystal
P-dbn_e > n_o at every tabulated wavelength (0.45-4.0 um) in this dataset: LT is weakly positive uniaxial here, unlike LN.
LiTaO3, composition not stated (comparison material)1965 bulk crystal
P-dbn_e > n_o at every tabulated wavelength (0.45-4.0 um) in this dataset: LT is weakly positive uniaxial here, unlike LN.
LiTaO3, composition not stated (comparison material)1965 bulk crystal
P-dbn_e > n_o at every tabulated wavelength (0.45-4.0 um) in this dataset: LT is weakly positive uniaxial here, unlike LN.
5 mol% MgO-doped congruent LiNbO3 (MgO5)
C5 mol% MgO-doped congruent LiNbO3 (MgO5)
C5 mol% MgO-doped congruent LiNbO3 (MgO5)
CStoichiometric or near-stoichiometric LiNbO3 (SLN)near-stoichiometric
P-compStoichiometric or near-stoichiometric LiNbO3 (SLN)labelled 'stoichiometric' (1967 crystal)
P-compConflicts with Volk & Wöhlecke 2009 near-SLN values.
Endpoints
curl -s https://lithium-niobate.com/api/v1/properties/refractive-index-o.json
This page carries the same records as schema.org Dataset JSON-LD. All endpoints: API.